dc.description.abstract |
Road construction often focuses on the use of conventional materials. Due to the depletion of these conventional materials, this
cannot be always true. To overcome such problems, several alternative construction materials have been proposed as sustainable
solutions. Tus, this study has investigated the potential use of volcanic ash (VA) as an alternative fller material in hot mix asphalt.
Te investigation has used laboratory scale and purposive sampling method for sample collection. Te plastic index and specifc
gravity of volcano ash are 0.92% and 2.44, respectively. Te chemical composition analysis indicated that VA is a class-N
pozzolana material. Maximum stability of 11.38 kN was obtained at full replacement of volcano ash. Te tensile strength ratio of
the mix at full replacement of CSD and volcanic ash is 82% and 98%, respectively. From the fatigue resistance analysis, the
probable failure of pavement constructed with the mixture containing VA could be improved from 16600 to 14400. Due to its
rough surface, VA has better bonding ability with bitumen compared to CSD. Te mix prepared from VA has less deformation
tendency than that prepared from CSD. |